| Dielectric strength | Approximately 15–30 kV/mm for many cured, unfilled or filled epoxy systems | Indicates resistance to electrical breakdown through the material. The measured value is strongly affected by specimen thickness, defects, moisture, and test conditions. | ASTM D149; IEC 60243-1 |
| Volume resistivity | Often about 1014–1016 Ω·cm at room temperature when dry | Higher volume resistivity generally means lower leakage current through the insulation. Heat, absorbed moisture, contamination, and aging can reduce it. | ASTM D257; IEC 62631-3-1 |
| Relative permittivity (dielectric constant) | Commonly about 3.5–5.0 at 1 MHz, depending on formulation | Affects capacitance, electric-field distribution, and signal behavior. Lower values may be useful in some high-frequency designs, but must be assessed at the operating frequency. | ASTM D150; IEC 62631-2-1 |
| Dissipation factor (tan δ) | Often approximately 0.005–0.03 at 1 MHz for general epoxy systems | Represents dielectric energy loss. Lower loss can reduce heating in AC and high-frequency applications; the value changes with frequency, temperature, and moisture. | ASTM D150; IEC 62631-2-1 |
| Glass-transition temperature (Tg) | Approximately 80–180°C across common cured epoxy formulations | Above Tg, stiffness and dimensional stability typically decrease, and electrical properties may shift. Select a formulation whose Tg provides margin over the maximum service temperature. | DSC: ASTM E1356; DMA: ASTM D7028 |
| Water absorption | Often around 0.1–1.0% by mass after 24-hour immersion, depending on formulation and specimen | Absorbed water can lower resistivity and dielectric strength and increase dielectric loss. Humidity conditioning may be more representative than a dry, as-cured test. | ASTM D570; IEC 60068-2-78 for damp-heat exposure |
| Comparative tracking index (CTI) | Can span roughly 175–600 V across epoxy compounds; formulation-specific | Assesses resistance to surface tracking under a specified contaminant test. It helps inform creepage-distance design but does not replace required product or safety standards. | IEC 60112; UL 746A |
| Thermal endurance and aging | No single universal value; the applicable temperature rating depends on the complete insulation system and aging evidence | Long-term heat exposure can embrittle or chemically degrade insulation and change its electrical performance. A short-term Tg or heat-deflection value is not, by itself, a service-temperature rating. | IEC 60216; application-specific thermal aging and electrical testing |
| Cure quality and void content | Process-dependent; specify cure schedule and acceptable void or defect limits for the component | Incomplete cure, cracks, inclusions, and air voids can concentrate electric fields and promote partial discharge or premature breakdown, especially in high-voltage parts. | DSC or supplier cure validation; visual or imaging inspection; partial-discharge testing where applicable |